Melting Points of Polymers
Polymer Name |
Tm1 (°C) |
Poly(acrylonitrile), syndiotactic | 321 |
Poly(6-aminocaproic acid) | 224 |
Poly(trans-butadiene), 90% trans - 7% vinyl | 47, 89 |
PoIy(1-butene), isotactic | 124 |
Poly(caprolactam) | 222 |
Poly(decamethylene adipamide), Nylon 10,6 | 235 |
Poly(decamethylene sebacamide), Nylon 10,10 | 202 |
Poly(etheretherketone), PEEK | 357 |
Poly(ethylene adipate) | 63 |
Poly(ethylene oxide), PEG | 66 |
Poly(ethylene terephthalate), PET | 264 |
Poly(ethylene), PE | 141 |
Poly(hexamethylene adipamide), Nylon 6,6 | 272 |
Poly(hexamethylene sebacamide), Nylon 6,10 | 224 |
Poly(hexamethylene suberamide), Nylon 6,8 | 236 |
Poly(methyl methacrylate), isotactic | 144 |
Poly(methyl methacrylate), syndiotactic | 200 |
Poly(methylene oxide), POM | 172 |
Poly(4-methylpentene) | 243 |
Poly(propylene), isotactic | 179 |
Poly(styrene), isotactic | 242 |
Poly(styrene), syndiotactic | 276 |
Poly(tetramethylene oxide), PTMO | 41, 60 |
Poly(trans-1,4-butadiene) | 98, 144 |
Poly(vinyl alcohol) | 231, 266 |
Poly(vinyl chloride), PVC | 220, 305 |
Poly(vinyl fluoride) | 199 |
Poly(vinylidene chloride) | 202 |
Poly(vinylidene fluoride) | 176 |
Poly(ω-undecanamide), Nylon 11 | 187 |